Tuesday, May 11, 2021

Pakspiny. Drawing Sliver Coiling. Drawing Coiling. Drawing Sliver coiler. Coiler Speed | High speed Automatic Coiler | .

Drawing Sliver Coiling

When coiling sliver into the can it is important to maintain: a smooth compacted sliver with low hairiness, fill the can in the correct manner and minimize dust / trash accumulations in the coiler tube. 

 

 


    

Ø  Coiler tube

The form of the coiler tube has been developed to enable the sliver to move with minimal interference into the can. The tube is normally made of stainless steel, which is wear resistant and suitable for most fibers. There are a very few exceptions in which the sliver is not compatible with the frictional characteristics of steel, and will not freely slide through the tube. In this case it may be necessary to use a brass coiler tube.The coiler tube and plate have to be selected to suit the sliver weight and the diameter of the sliver can. 

Ø  Coiler tube inside diameters

 To obtain a smooth and compacted sliver the coiler tube should be as small as practicable. If the tube diameter is too large for the sliver, the sliver will have a tendency to:

·         Be hairy,

·         create difficulties during withdrawal from the can,

·         have a reduced sliver cohesion.

·         detailed Rieter recommendations can be found in the machine manual

 

Ø  Sliver deposit

 Depending upon the sliver can size, the sliver is coiled either “over center” in cans 225 to 600 mm diameter or “under center” (some references use “onto the center”) in cans 800 to 1000 mm diameter.

Ø  Coiler settings

To maintain good quality coiling of the sliver, the following points of the coiler have to be correctly set:

Coiler speed depending upon material and sliver weight. The speed must not be excessive and stretch the sliver, nor too slow and lay the sliver unevenly in the can  location (eccentricity) to build a column diameter 10 mm smaller than the can’s inside diameter. This should be checked when the can is 75 % full,Can table speed to adjust the coil spacing so that the sliver coils are side by side, not overlapping and not spaced apart.Length of sliver in a full can must not be excessive. An overfilled can creates problems of sliver disturbance and scuffing which leads to drafting problems at the subsequent processes.

·         The can condition has to correct, damaged and out-of round cans cause many problems and a deterioration of sliver quality.

·         The cans must be the required size and set relative to the coiler plate.

·         The can spring length and pressure must be correct for the material being processed.

·         The coiling conditions have to be checked and, if necessary adjusted, with any change of: Sliver weight, - Material,

Coiler speed

Check coiler speed





 

 The coiler speed is too low. The sliver (1) is pulled to the outside of the coiler exit. This pushes the coils onto each other and the sliver tends to pull apart when being removed from the can.

The coiler speed is correct. The sliver (2) leaves coiler plate at back of the kidney-shaped.

The coiler speed is too high. The sliver is pulled to the inside of the coiler exit.

The sliver is stretched, the coils will be deformed and periodic draft faults may occur.

 

 

Ø  Correct coiler speed

 Coil diameter (A) is evenly round. Distance (a) between the coils (A) remains uniform around the can.The form of the sliver column (2) is evenly round and 5 mm clear of the can side (1)

  Coiler Speed Too Low

 The coils are too wavy.

The distance (a) between the coils (A) is relatively uniform.

The Diameter of the sliver column (2) is too large and is equal to or greater than the inside diameter of the can (1).

Ø  Coiler speed too high

 

Sliver coils (A) are out of round and are not consistent. The coils are drop shaped with the tip pointing toward the can inside wall (1) The distance (a) between the coils varies from one coil to another. The sliver column (2) is out of round. The sliver column (2) is too small and the clearance between the column and the inside of the can is more than 5 mm.

 

Coiler speed correct




 

Coiler speed too low

 

 


Coiler speed to high


 

   Sliver coils per can revolution


 

The sliver coils per layer is obtained by dividing the speed (rpm) of the coiler by the rotational speed of the can table. With larger diameter cans the number of coils per layer increases to maintain optimal coiling and can filling.

nD = Relationship of coiler rpm to can table rpm

nD = coiler rpm

can table rpm

The following can be used as a guideline

  • Ø  Can eccentricity

     The outside diameter of the sliver column is primarily established by the relative positions of the centers of the coiler and the can table. This distance is referred to as the eccentricity. If the can table is moved to reduce the eccentricity the sliver column will be reduced, and conversely the column will be increased if the table is moved to increase the eccentricity. The setting of the can table eccentricity is normally not changed.

    However, it may be necessary to make a re- adjustment if there is a change to fibers of greatly different bulk characteristics, such as cotton to acrylic fibers.

Pakspiny. Sliver Feed to the scanning rollers. Drawing Draft. Drawing Break Draft. Drawing Roller. Draw scanner Roller

 

   Sliver feed to the scanning rollers

It is essential that sliver funnel and the scanning rolls of the auto leveler are very carefully set. An incorrect setting can cause cutting of the fibers, sliver tags and highly compressed sliver fringes that are not subsequently drafted.

·  The funnel should be correctly located and be 0.5 -1mm from the scanning rolls.

·  The funnel must be centered relative to the scanning roll groove.

·  The tongue and groove  onents must not make contact with each other.

·   The sensing scanning roll must not touch the funnel.

The clearances between the scanning rolls should be checked at ¼ turn positions to be sure that they are correctly aligned.Clearances should be checked above and below the tongue as well as between the tongue and inside of the grooved roll Sharp edges of the scanning rolls can cause cutting of fibers.

This shows up as an increase in short fiber content after drawing. Additionally synthetic fibers can be fused. The sharp edges should be polished away by using fine “Scotch Bright” or similar polishing material. The pressure on the scanning roll should be carefully adjusted to suit the processing speed and the material being drawn. If there is scanning roll vibration the pressure should be increased incrementally. For bulky coarse synthetic fibers it is sometimes necessary to increase the pressure For polyester the pressure is usually light.

Check that the scanning roll assembly screws do not touch the table. This is a problem if a change is made to smaller scanning rolls and using the same length screws. Clean the funnel. There should be no contamination, burrs or rough places.


Funnel and scanning rolls

 


 


 

      Scanning rollers to drafting system

Ø  Sliver tension

 

The sliver tension must be carefully adjusted to avoid sliver stretching but to be sufficient to cause the slivers to spread after the high compression of the scanning rolls. High tension will cause irregular stretch that cannot be corrected by the auto leveler. With combed cotton the piecings can be disturbed and the autoleveler will not function correctly. Reduce the tension until the slivers are slightly loose and then increase the tension one step. The sliver should not drag on the table.

 

Ø  Sliver spreading

 

When the slivers leave the scanning rolls the material is very compacted and has to spread to a “side by side” condition prior to entering the drafting system. Slivers must not roll and cross each other.

The sliver guide bars L1, L2, L3, and L4 must be set so that the slivers are:

•  in the center, uniformly next to each other, without gaps between the slivers, no slivers crossing,

 

Ø  without rolling and twisting.

 In addition to the sliver tension, the relative heights of the sliver guide bars influence the spreading action. The convex shape of the guide bars helps in the spreading action. Initially set the bar heights with L1 in the high position, L4 below the back roll of the drafting system, L3 and L4 as shown in the diagram. If the spreading is excessive and the slivers are moved apart then lower L3 or raise L2 The sliver path must be as that shown in the diagram, otherwise the correct leveling and drafting functions will be disturbed. 

Ø  Drafting

 Sliver path through the Drafting System

 The drafting system is basically 3 over 3 with an additional “Deflection” roll (7) on the delivery roll to direct the sliver toward the coiler.

 The top rolls are numbered (1, 2, 3) and corresponding bottom rolls are, - back roll (4), middle roll (5) and delivery roll (6).

There is a pressure bar (8) located between the top rolls 2 and 3 to help control the fibers in the main draft zone.The fundamental settings of the drafting system are the roll distances and the draft distribution. Each greatly influences the quality of the delivered sliver.

Ø  Critical factors affecting the drafting action

 •  Roll settings, draft distribution, roll pressure, speed, top roll cot condition

 removal of dust, fly and clearer waste.

Ø  Roll setting

 Drafting roll distances have to be set as close as practicable:

To control the short and floating fibers, Not so close as to break the longest fibers, nor Not so close as create high drafting forces and over control.

The roll setting has to be optimized according to:

•  Staple length, ( 2.5% on HVI or AFIS and 1.0% on the Peyer AL-101) fiber orientation,

Ø  sliver weight

  fiber crimp, bulk and cohesion. The number of fiber hooks are decreased and the degree of fiber orientation is increased each drawing process. Therefore, it is necessary to set the roll spacing with this in mind.

Ø  Setting tip

 From the practical setting perspective, the main draft rolls should be set first, followed by the setting of the break draft zone. Any change of the distance between rolls (5) and (6) automatically changes the distances between rolls (4) and (5). Consequently, a change of setting of the main draft zone must be followed by an adjustment of the break draft rolls.

The converse is not so. A change of the distance of the break draft zone does not change the positions of rolls (5) and (6).The main draft zone roll – setting (H V D)

• The main draft rolls have an actual minimum setting of 35.5 mm, which is used for all fibers with staple length shorter than 27 mm.

 

• For fibers of staple length 27 mm or longer, the rolls are Normally set at 8 ….10 mm over the 2.5% length value. Break draft zone - roll setting (V V D)

 • The break draft roll setting is dependent upon the condition of the supplied sliver. The maximum and average staple lengths, the degree of fiber orientation, the fiber hooks, the drafting resistance, and the draft distribution all have an influence on how close the rolls can be set. A simple test for the break draft resistance is to use a1 or 2 mm feeler gauge and push it between the first and second rolls into the slivers. The fibers should yield but with resistance. The rolls are too close if the slivers do not allow the feeler to be pressed through. Closest roll setting is 36 mm Common roll settings range from 10…15 mm over the 2.5% staple length.

Ø  Draft distribution

 • The total draft is established by the total mass of the input material and the mass of the output sliver.

  The calculation is:

Total draft  (V) = Input mass ÷ Delivered mass

The total draft is performed in two stages. The first step is the “Break Draft” (V V), which prepares the slivers for the “Main Draft” (V H) Break draft zone - Draft (V V ) The function of the break draft in the draw frame is to pre tension the slivers and remove the sliver crimp so that the fibers presented to the main draft zone are controlled. The normal range is 1.16 to 1.41, but with polyester for sewing thread and crimped acrylic the break draft can be up to 1.70. The break draft in the first drawing passage is usually higher than that of the second passage because the card sliver has a lower level of fiber orientation. The evenness tester diagram and spectrogram should be used as a guide in setting the draft.

The following observations can be made:

 Breaker drawing requires higher break draft than subsequent drawing processes.

 Warning: Roll settings that are too close will result in over control, which can be seen as “spikes” in the evenness diagram. These spikes cause thick and thin places in the yarn. Finisher drawing requires more open settings and a lower break draft. Man made fibers require higher break drafts than cotton.Finer fibers, cotton or man made, require higher break draft than coarser fibers. When the total draft has to be relatively high (7 to 10) thebreak draft has to be increased to keep the main draft in the desirable range. When processing short fibers the break draft should be low. 

Ø  Main draft zone – Draft (HV)

 The main draft is established by the total draft and the break draft .The total draft is set by the overall processing system and usually has to be accepted. However, for high quality products, it is recommended to limit the draw frame draft to less than eight (8), which means the main draft will be between 3.5 and 5.5.

•  The best main draft settings are dependent upon the materials being processed, and the following points generally apply:

 

 Comber noil                   HV – 3.8,

 short carded cotton         HV – 4.75,

 carded cotton                 HV – 5.2,

 combed cotton               HV – 6.1,

 Egyptian combed cotton  HV – 7.1,

 cotton /MMF Blends        HV – 6.2,

 viscose                          HV – 6.3,

 acrylic (crimped)            HV – 5.2,

 polyester (crimped)        HV – 6.0,

 polyester (sewing thread) HV – 3.7,

 polypropylene (…..den)    HV – 6.1

Ø  Roll pressure

 The top rolls are pressure - loaded against the bottom rolls to grip the fibers between the rolls and to increase the fiber bundle pressure in the drafting zone. The pressure should not be excessive, but has to be sufficient to maintain a consistent drafting action.

The following points should be noted:

Rolls 1, 2, and 3 are pre set to 320 N, Deflection roll 7 is preset to 200 N,

For conditions of high drafting forces, such as, low draft ranges, heavy sliver weights or fibers that have a strong drafting resistance the top roll pressure has to be increased to:

Top rolls 1 and 2 to 440 N,Top roll 3 to 320 N,Deflection roll 7 remains at 200N.

When the top roll pressure is increased the effective nip zone is extended reducing the distances between the nip points. To compensate for this, it may be necessary to increase the draft roll settings by 1 or 2 mm. Increasing the roll pressure increases the temperature or the rolls, Lifetime of top rolls is reduced, Top roll deformation will occur if roll pressure is left on when the machine stops With the pneumatic top roll loading system, the pressure is automatically released. This prevents the formation of flat spots on the cots.

Pressure on Drafting System:

 Speeds of the draw frame have been progressively increased. In most cases the maximum speed of the draw frame is limited by:

• The running condition, which is fiber dependent, or

• The sliver quality that can deteriorate as the speed exceeds optimal levels.

• Normally, the draw frames are run at speeds below the maximum rate because the cost of drawing is a relatively small component of the overall spinning costs.

 Effects of excessive speed

 • Increased top roll laps,

• Roll temperatures exceed the tolerance of some man made fibers,

• Increased machine stops and reduced efficiency,

• Deterioration in sliver quality,

• Reduced lifetime of the cots,

• Overheating of the bearings,

• Guide to maximum draw frame speeds.

 The following chart is taken from the sales documentation and represents the delivery speed expectancies of current draw frames. It should be emphasized that speeds approaching the maximum speeds can only be attained when all conditions are optimal.


Pakspiny. Drawing Machine Element. Drawing Creel Setting. Finisher Drawing Creel Setting.

  Drawing Machine Element

  • Ø  Sliver feed

 The running performance of the material in the creel is critical to the draw frame efficiency and the delivered sliver quality. Operator practice and machine set-up have to be carefully monitored.

  • Ø  Creel height

 Creel height should be sufficient to allow a sliver balloon to develop between the top of the material in the can and the creel guide. A minimum clearance of 500 mm is preferred. Avoid “dragging” the slivers across the top of the cans. Sliver stretching occurs which is very undesirable. Additionally, slivers dragging over the can edge disturbs the sliver and creates defects which will be seen in the yarn.

  • Ø  Block creeling

 If the length of sliver in the cans in the draw frame creel is consistent, block creeling is frequently preferred. Draw frame efficiency is increased because of reduced stops due to sliver run-out. With no sliver splices due to creel can changes, the delivered sliver is of a higher quality and creates fewer stops in the downstream processes. Bad splicings in the creel can create chokes at the condenser, or undrafted pieces in the delivered sliver that cannot be drafted in ring, air-jet or Vortex spinning. Removal of the creel splicings after drafting produces the best sliver quality. With block creeling, the creel sliver splicings are run through the draw frame into the can and then removed from the top of the can.

  • Ø  Random creeling

 When a plant selects to random creel, the creel sliver splice is not normally removed. Therefore the operator has to be taught how to make a splice, which will be sufficiently strong to be transported through the creel, but be soft enough to be drafted out in the draft zone. Avoid damaging sliver by reaching down the side of the can to find the sliver tail when it is to be spliced to the sliver in the following can. If a sliver end is laid into an adjacent sliver and that is then used to pull the sliver end through the machine, care must be taken to ensure that the slivers are correctly arranged in the rake.

Some operators are required to pull the new sliver over the creel through the rake and the fold the end into an adjacent sliver. This system can work well as long as the sliver and the end are not compacted and difficult to draft.

  • Ø  Sliver splicing technique

 Prepare the sliver ends to be spliced by removing a Vee shaped portion about 2 to3 inches long. Overlap the Vee portions of each sliver to form a relatively uniform joint. Work the fibers in the joint by lightly pulling sideways to create an integrated splice. Squeeze the joint together and roll slightly between the palms of the hands to develop some sliver cohesion. Do not roll and twist the splice, or wet the palms of your hands to make the slivers stick together. The splice should be draftable and not cause a hard slub.


  • Ø  Static creel

In the static creel the slivers have to be pulled from the cans over the guides and into the draw frame. It is very important to minimize drag angles over bars and guides. It is particularly bad when the sliver is pulled through a ring or over a bar and there is an angle of wrap of almost 180 degrees. Position the cans to permit the sliver path to be as direct as possible. Remove all rough places that cause slivers to hang. Avoid placing cans so that the sliver balloons become entangled.

  • Ø  Power creel

 The power creel is provided to reduce the tension forces in the sliver. The sliver is pulled up from the can by a lifting roll and is then pulled to the feed roll. The drive to the lifting rolls can be varied so that there is only a slight sliver tension and no overfeed. To find the preferred tension, reduce the tension in the creel until the sliver is slightly overfed and then increase the tension by one small step. As the speed of the machine is changed or the material is change it is usual to have to adjust the creel tension.

  • Ø  Sliver in-feed and jockey rolls

 The jockey rolls driven by the In-feed rolls feed slivers to the drawframe. Normally there are two slivers under each jockey roll. If a sliver is missing the metal jockey roll should touch the in-feed roll and activate the stop motion. The jockey rolls must be free to move. There should be 1.0 mm clearance between each stop pin and the jockey rolls. When roll clearers are provided for the sliver in-feed it is important that they be kept clean. 


 

Adjustment of Jockey Roll

  

 Ø  Sliver tension

 It is important that the sliver tension should as low as possible but it should control the sliver movement. Reduce tension until slivers are loose and then increase the tension by one step. Check that slivers do not roll and cross as they move through the machine. Slivers should not be stretched.

  

Pakspiny. Function of draw frame. Draw Technological Function. Draw frame working principle. Introduction of draw frame. Draw frame working principle.

     TECHNOLOGICAL FUNCTIONS

    Introduction

  Every aspect of the drawframe and the movement of the fibers can have an impact on the technological aspects of the delivered sliver. The challenge is to produce fault free high quality sliver at near maximum production speeds. The overall sliver quality is determined by:

The type and quality of the fibers being processed,

The machine condition and process control of previous operations,

The processing system variations such as combing, multiple drawing

 steps, and the blending techniques for different fibers.

The results will be different for each of the many variables, but each will have an optimal drawing set up.

 

Unfortunately, any defects in the sliver leaving the finisher draw frame are going to cause subsequent processing stops or a yarn / fabric defects. The primary problems are associated with either the machine condition operator practice or the machine settings and include:

Drafting conditions that create uncontrolled sliver thick/thin places, clearer waste from the drafting rolls and drafting waves.

Uncontrolled sliver stretching in the coiling action, or any sliver stretching that cannot be removed by an auto leveler. 

Sliver tension, throughout the machine should be low. Establish the tension by finding the point at which it is just too low and then increase it by one step.Sliver contamination due to the release of accumulated dust and fly.Sliver tags produced by rough spots in the sliver path or by defective cans. Damaged sliver caused by bad operator handling techniques..


 

 

   Influence of fibers

The basic rules are:

Long, fine fibers of uniform length can be drafted at the high end of the draft range, carded cotton and blends should be limited to a maximum draft of eight.

With very short regenerated fibers the draft should be limited to four, and only one process of drawing. Multiple drawing processes create a very high level of drafting waves. Additionally, These fibers normally have to be run at speeds below 400 m/min.

 

Synthetic fibers with high fiber-to-fiber cohesion require higher drafting forces, create more heat and in general have to run at slower speed, in the range of 400 to 500 m/min.

The fiber finish on some synthetic fibers can create a finish build up on the machine, in the coiler tube and on the coiler plate. Care has to be taken to keep the machine clean.

Some bulky synthetic fibers need special components to run well. Check with the business unit if this is a problem.

 

   Number of drawing processes

 The number of drawing processes is normally established by the technological requirements because the cost of drawing is relatively low. However, there is always pressure to reduce processing steps to remain competitive.It is well established that the card produces a sliver containing both leading and trailing hooks that have to be eliminated prior to high draft ring spinning. This is normally done by using two passages of drawing

 

   Single process drawing

 (Single process drawing can be used where the spinning process is not sensitive to fiber hooks or poor fiber orientation. 

These include:The spinning of coarse counts from blends containing very short fibers such as comber noil, regenerated fibers or gin motes.

An additional drawing process is not used with this type of material because it can create problems of drafting waves and reduced sliver cohesion.

Rotor spinning of coarse and some medium count yarns. Fiber hooks and fiber orientation do not greatly affect the spinning process but there will be a loss of strength by using only one process of drawing. This is not a problem for many pplications.

Coarse counts spun from synthetic fibers. Some carpet and upholstery yarns are produced on both ring and rotor spinning systems.


 

   Two process drawing

 The conventional short staple process, for “carded” yarns of cotton, man made fibers and intimate blends, includes two drawing processes.The primary reasons for two processes are:To reduce the number of fiber hooks in the sliver,Supply roving, with the majority of hooks trailing, to the ring spinning, To improve the degree of fiber orientation in the liver,To enable blending through doubling to improve yarn consistency,To gradually reduce the sliver weight from the card sliver to that needed by the roving or spinning machines.

 

   Drawing for combed yarns

 In the modern combed yarn spinning, there are three drawing operations:

First passage of preparation drawing is used to draw card sliver and produce sliver that can be wound onto laps for the comber.

The second drawing operation occurs at the comber to reduce the sliver weight. Relatively high drafts are needed at this stage and the drafting zone is very robust. The drafting system is normally a 3 over 5 roller arrangement to clearly separate the fiber control function of the break draft zone and the main draft zone.The third drawing operation is performed on the finisher drawframe.

The comber eliminates most of the fiber hooks, hence the remaining functions of the drawframe are to produce a very uniform sliver of the required weight. This “one process drawing” after combing has been made possible by the successful use of the RSB autoleveler drawframe.




 


   Three process drawing for drawframe blends

 When blending different fibers at the drawframe, multiple processes have to be performed to produce a homogeneous finished sliver. This is usually necessary for ring spinning.

An exception is in rotor spinning in which the yarn formation steps separate the fibers and reassemble them in the rotor to produce a well lended yarn. In some rotor spinning plants only two drawing processes are used)


   Three process drawing for air jet and Vortex spinning

 Three processes of drawing are normally used to prepare sliver for MJS and MVS.

The spinning machine drafts directly from sliver with drafts over 150. The fibers in the sliver have to be individualized and very well oriented. With three processes of drawing, the spinning machine functions more efficiently.

The machines need light sliver weights to be able to spin medium and fine yarn counts. Slivers in the range of 35 grains/yard are not unusual. Three drawing steps are helpful in converting relatively heavy card sliver into light finisher drawing sliver.

The processing of combed cotton for MVS is a challenge because spinning results are good with only one process of autoleveler drawing after the comber. This requires drafts much higher than normal range. 


  Sliver quality

 As frequently mentioned throughout the chapter on Settings, the sliver quality is of primary importance. The sliver quality is normally judged by consideration of the Test Lab Data produced under controlled conditions. 


   Sliver weight

 The weight of the sliver is usually measured in g/m or grains/yard. Obviously, the shorter the length of the individual samples, the more the variation is revealed. For example, it is not recommended to reel long lengths of sliver to check the autoleveler function.


The following checking procedures are suggested.

Delivered sliver weight of a machine - 5 x 10 yd (m).

( Not consecutive lengths.) Machine to machine sliver weight control – 5 x 10 yd (m) lengths from each machine. “Sliver Test” for leveling intensity…3 x 10 yd (m).



Care has to be taken when manually preparing and cutting lengths of sliver. The sliver is easily stretched and if different operators perform the task there can be manual errors introduced.

When a reel is used, care should be taken to prevent sliver tension variations that could cause uncontrolled sliver stretch.


   Sliver evenness CV%

 The evenness is normally measured by passing the sliver through a measuring head that records a capacitive signal measuring the mass of every 12 mm of sliver length. The values are represented in a continuous chart that shows the variation of the sliver above and below a mean value. This chart is called the “Diagram” in this text.

The data is used to calculate the mathematical value of mass variation known as the coefficient of Variation (CV%). The lower the CV%, the more uniform is the sliver.

Additionally, a Spectrogram is produced that shows the periodic occurrences of variations.

It is normal for customers to request the lowest possible sliver CV%. To do this, the draft distribution has to optimal and the roll settings close. These tight roller settings tend to:

Over control the sliver and break the longest fibers, Reduce the yarn strength,Increase the ends down rate in spinning.Create small “spikes” visible in the evenness diagram that cause Increased thick places in the yarn.


 

 Evenness diagram of a sliver with a low CV% but with spikes in the diagram

 



The ultimate judgment of the best CV% can be made only by considering the

 Diagram, the Spectrogram, the processing performance at roving and spinning

 and the yarn quality. Unfortunately a considerable length of time is needed to

 perform these extensive evaluations; hence, the customer should be encouraged

 to assist.


 

   Effects of tight roller settings

 

Effect of drawframe roller spacing on yarn quality

Ne 30/1 – 100% combed cotton ring yarn. (41 mm staple)

 

Too tight

(lowest CV% 2.7%)

Optimized setting

(CV 3.0%)

Roller spacing (HVD/VVD)

40 / 46

42 / 47

Single end strength

420 g

412 g

Strength variation -Vo

7.8%

6.2%

Single end elongation

6.5%

6.5%

Elongation variation -Vb

2.4%

1.9%

 

Uster CV %

12.2

11.7

Thins

0

1

Thicks

16

10

Neps

11

10

 

Classimat minors

80

28

Majors and long thicks

22

2

 

ITT quality index

(higher is better)

137

146

 

 

Recommendation – In many cases the best settings are found to be:

 Roller distances for lowest CV% but with the main draft zone opened up by 1 - 2 mm, and the break draft zone opened 2 – 4 mm.


 

   Spectrogram

 The spectrogram is extremely important in judging the sliver quality in that the periodic mechanical faults and the sliver irregularity waves can be seen. Additionally, if the leveling action point is not correctly optimized, a hump in the spectrogram will be visible somewhere between 35 cm and 50 cm.




 

  
 

 The appearance of sliver can indicate the quality, and is an important element in judging how well a machine is performing.

 

 

When the can is full and doffed the following points should be observed:

The sliver should not be “scuffed” from over filling. This leads to matted fibers that are difficult to draft in subsequent processes. DO NOT OVERFILL the cans.

If the sliver is folded during the coiling action the tension is too low.

Fiber tags on the surface of the sliver usually means that the coiler tube or coiler plate has a rough place that needs to be repaired or replaced.

Trash accumulations in the top coils, sometimes referred to as “mice”, are due to trash collecting in the coiler tube during running and being released as the coiler slows down at a stop. The coiling tension should be reduced slightly to enable the sliver to have a more complete contact with the coiler tube.

 

   Sliver cohesion

 If the sliver has low strength, the trumpet, calender roller pressure and coiler tube inside diameter should be checked to see if they are correct for the sliver weight and material being processed.

With combed cotton, the strength of the drawn sliver is influenced by the piecing produced at the comber. Many times the optically best piecing seen in the combed web is too delicate for the subsequent drawing steps. It is suggested that heavier overlaps at combing produce a stronger sliver. The associated mass increase can be subsequently corrected by the leveling action of the auto leveler draw frame. 

Finisher Drawing Uster Test . Finisher Drawing Quality Check .Finisher Drawing Diagrams & Spectrograms Faults.

 Spinning Mills Machine. Finisher Drawing Uster Test. Finisher Drawing Quality Check. Finisher Drawing Diagrams & Spectrograms Faults. P...